E309 Ss Wleding Rod

E309 Ss Wleding Rod

1. Chemical Composition (Mass Fraction, wt%) 2. Mechanical Properties (Room Temperature) 3. Physical Properties (309 Base Metal)
Send Inquiry
Product Introduction

 

1. Chemical Composition (Mass Fraction, wt%)

Category C Si Mn P S Cr Ni Mo Remarks
E309-16 (AWS) ≤0.15 ≤1.00 0.5–2.50 ≤0.040 ≤0.030 22.0–25.0 12.0–14.0 ≤0.75 -
E309L-16 (AWS) ≤0.04 ≤1.00 0.5–2.50 ≤0.040 ≤0.030 22.0–25.0 12.0–14.0 ≤0.75 Low carbon for intergranular corrosion resistance
E309H-16 (AWS) 0.04–0.08 - - - - 24.0–25.0 12.0–14.0 - Higher high-temperature strength
ER309 (AWS) ≤0.12 0.3–0.65 1.0–2.5 ≤0.030 ≤0.030 23.0–25.0 12.0–14.0 ≤0.75 For gas metal arc welding (GMAW)
ER309L (AWS) ≈0.02 ≈0.42 ≈1.88 ≤0.020 ≤0.001 ≈23.0 ≈13.7 ≤0.08 Typical composition
309 Base Metal (ASTM A167) ≤0.20 ≤0.75 ≤2.00 ≤0.045 ≤0.030 22.0–24.0 12.0–15.0 - Austenitic stainless steel

2. Mechanical Properties (Room Temperature)

Category Tensile Strength (Rm) Yield Strength (Rp0.2) Elongation (A) Hardness Remarks
E309-16 Deposited Metal ≥550 MPa - ≥30% - As-welded condition
E309L-16 Deposited Metal ≥520 MPa - ≥30% - As-welded condition
E309H-16 Deposited Metal 552–593 MPa (80–86 ksi) 462–490 MPa (67–71 ksi) 38.2–41% - CO₂ shielded
ER309 Deposited Metal ≈601 MPa (≈87.2 ksi) ≈400 MPa (≈58.0 ksi) ≈40% - Typical value
309 Base Metal (Annealed) ≥517 MPa (≥75 ksi) ≥207 MPa (≥30 ksi) ≥40% ≤RB95 Conforms to ASTM A167

3. Physical Properties (309 Base Metal)

Item Value Unit Remarks
Density 8.00 g/cm³ -
Elastic Modulus 200 GPa -
Coefficient of Thermal Expansion (20–100°C) 14.9 µm/m·K -
Thermal Conductivity (20°C) 15.6 W/m·K -
Melting Point 1400–1455 °C -